My pressed powder crumbles or caps after I added kaolin. What went wrong?

Usually too much kaolin, or too little binder to compensate for it. Calcined kaolin is a strong oil absorber, so it takes binder out of circulation — the pan is under-bound even though the binder percentage on paper has not changed.

Two things to try. Raise the binder by 10–20% relative to the kaolin you added, and bring in a small amount of a platy material such as mica to restore the press strength that kaolin alone does not provide. Kaolin improves hardness up to a point and then reverses, because past roughly 15–20% there is not enough binder left to cover the increased surface area.

If the compact is capping rather than crumbling, look at the press instead. Too fast a cycle and an uneven fill produce capping that no formula change will fix.

Regulatory status — Kaolin (calcined) INCI KAOLIN · CAS 1332-58-7
MarketStatusBasis and conditions
EU Permitted CosIng listed; no Annex restriction — Crystalline silica is classified Carc. 1A by inhalation, but cosmetic kaolin is a hydrated aluminium silicate, not free crystalline silica; the respirable crystalline silica content belongs in the specification.
UK Permitted No Annex restriction
US Permitted No ingredient-level restriction
China Permitted IECIC
Japan Permitted General cosmetic ingredient
ASEAN Permitted ACD, no Annex entry
Korea Permitted MFDS cosmetic ingredient standard
Canada Permitted Hotlist: not listed

Swipe the table sideways for the full basis column →

Watch: None. Note that "crystalline silica" restrictions apply to free crystalline silica, not to kaolinite.