The powder will not disperse in our system and leaves specks. Is it the material or the process?

An isolation test settles it: disperse this powder alone in the same medium, with no other powders and no other additives. If specks remain, the cause is the powder itself (hard agglomeration or moisture). If they disappear, the cause is the formula or the process.

Three common formula causes: adding powder into the oil phase instead of oil into powder; a dispersant mismatched to the surface treatment (silicone-treated powders run more freely in non-polar systems); and skipping the wetting stage by heating too early.

Two common process causes: insufficient dispersion tip speed (same time at half the tip speed gives a very different result), and incomplete vacuum deaeration, which traps particles inside bubbles.

Send us the isolation test result plus the formula composition (redacted is fine) and we can identify which side the problem sits on.